Gas Firing 2016.02.20 Comments and Notes

This firing of the kiln went too long, resulting in Orton cone 11 flat.  Ideally, it would be cone 11 touching, then sagging a bit.

Upon unloading the kiln this morning, one thing was immediately apparent: the right side was far more reduced than the left. Yellower glazes and more slumping. Even on the left side there was some slumping, because of the excessive temp., and because of the clay which contained some low temp high iron clay to help seal the ware against leakage.

Left side, sagging only slightly, white surface.
Left side, sagging only slightly, white surface.
Right side sagging badly, white glaze turned yellow.
Right side sagging badly, white glaze turned yellow.

Chosen Karatsu came out pretty good, but the white was on too heavy, running down the pots too much.  It still came out looking ok because of the clay.

Most of the teabowls warped or sagged, so I only get to keep 2 or 3 of the 15. This is why teabowls are expensive, kids…IMG_3399 IMG_3398

All in all, not a bad firing, but need to adjust clay bodies, and pay closer attention to cones. Also, figure out the over reduction on the right side. It might be that one burner that sounds a bit off.

Kakewake CG bowls
Kakewake CG bowls
guinomi, need more sand in the clay
guinomi, need more sand in the clay
crystals, only grew on the right side, where reduction was strongest.
crystals, only grew on the right side, where reduction was strongest.
cylindrical tea bowls
cylindrical tea bowls
yunomi
yunomi
shells on feet
shells on feet

IMG_3437

saggared and much improved.
saggared and much improved.
porcelain, saggared
porcelain, saggared

IMG_3464 IMG_3463 IMG_3462 IMG_3460 IMG_3459

 

2 thoughts on “Gas Firing 2016.02.20 Comments and Notes